Results of atmospheric and laboratory corrosion testing are presented for a new hot dip aluminum-zinc alloy for the corrosion protection of steel sheet, developed and available since 1972. The coating comprises 55% aluminum, about 1. 5% silicon, with the balance zinc, and has primarily a two-phases structure after solidification on the steel surface, consisting of a major dendritic aluminum -rich phase, and a minor interdendritic zinc-rich phase. Corrosion test results show that the coating is 2 to 4 times as corrosion resistant as galvanized coatings of equal thickness, and provides galvanic protection to steel at cut edges of uncoated areas. Examination of the coating microstructures before and after testing, and measurement of mass loss rates and electrode potential changes in solution indicate that in the initial stages of exposure, the zinc-rich phase corrodes preferentially, at a lower rate than galvanized coatings because of the smaller area of zinc exposed. After this phase has been depleted, the corrosion characteristics become those of the aluminum-rich phase, resulting in a decrease in the corrosion rate. Galvanic protection is provided by either the zinc-rich of both phases, depending on the chloride content of the environment.