A method has been worked out for the chlorination of chromite with CC14 vapour, which can be used either for selective action on the iron constituent or for the complete chlorination of both iron and chromium. Chlorination is inappreciable at 650°C At 700C., the chlorination of iron is more pronounced, and best results are obtained in two hours when 80% of iron is chlorinated but only a third of the Cr203 is affected, the Cr/Fe ratio of the residue increasing to 10.64 (from 2.9 of the original ore). Formation of Cr Cl becomes pronounced from 750oC. Virtually complete chlorination of Cr203 (and, of course, FeO) can be achieved in three hours at 850oC. Silica remains unaffected. Influence of several incorporates have been studied and probable mechanism of the reaction discussed.