Bulk ceramic samples with nominal compositions of (Er5Ba5)CuOy,y=6 to 7, (Er33Ba66)CuOy, and (Er33Sr66)CuOy, have been prepared by solid state reaction technique at 914C. The samples were simultaneously given heat treatment under identical conditions to avoid ambiguity in the preparation history. The samples had been characterized by optical microscopy, x-ray diffraction and low temperature resistivity measurements. Only one composition namely, (Er5Ba5)CuOy showed superconducting transition at 90.5 K with a transition width T= 1.5 K. Zero resistance state for the other two samples was not observed up to 77 K. Er-Ba-Cu-O system was found isomorphic with the Y-Ba-Cu-O and Ho-Ba-Cu-O system.