Nylon-6, 10 is prepared by an interfacial polymerization reaction between sebacoyl chloride (SC) dissolved in CCI4 and a hexamethylene diamine (HMD) sodium hydroxide solution. Different molar ratios of HMD: SC were applied to produce polymers of different molecular weights. The relative viscosities of the synthesized Nylon-6, 10 were experimentally determined. The intrinsic viscosities were computed and plotted against concentration, from which the limiting viscosity numbers were obtained. The molecular weight of the polymers for each molar ratio was calculated using the Mark-Howuink-Sakuracla equation. All molecular weight values obtained, except one, are in good agreement with literature. Also the results indicated that the degree of polymerization of Nylon 6, 10 is increased by increasing the ratio of HMD.