The radiolysis of poly (vinyl) chloride (PVC) in chloroform, carbon tetrachloride and dimethyl formamide was studied in air. A few samples without solvents were also studied under similar conditions to serve as blanks. A continuous decrease in intrinsic viscosity was noted in blank samples. Samples irradiated in carbon tetrachloride showed decrease in intrinsic viscosity upto 3.5 megarads. On further irradiation an increase was noted. In chloroform the intrinsic viscosity first increased gradually up to 5 megarads and later on the increase was very fast. Colour development in samples irradiated alone and in solvents was observed and this was attributed to conjugated structures. Thermal gravimetric study revealed better heat resistance in samples irradiated in chloroform and in carbon tetrachloride, the former being more thermally stable than the latter at lower dosages.