Cu-Mn substituted 18/8 type stainless steels excel the unsubstituted varieties in many respects such as cost, corrosion resistance, hardenability, machinability, toughness under cryogenic conditions etc. Ni is an indispensable constituent of Cu-Mn substituted 18/8 type steels. The substituted steels cannot afford to have less than 5% Ni, if the characteristics of structure, hot-workability, corrosion resistance and unsusceptibility to martensitic transformation are to be maintained as in normal 18/8 steels. In the present work, the base-composition selected for study contained around 17% Cr, 5% Ni, 1.5% Mn, 3% Cu, 0.07% C and 0.03% N. The effect of gradual additions of Ni from 5 to 7.8% indicated that corrosion resistance of the steels was improved, delta ferrite formation reduced, alpha-iron content decreased, Ms temperature depressed and hot-shortness suppressed. In fact, the austenite in the studied steels was stabilized by successive additions of nickel.