Electrical resistivity of powdered wood charcoal of different grain sizes thermally activated at temperatures 35C, 500C, 600C, 700C, 800C and1000C was determined into an applied pressure of 1931 lb/in2. No meaningful dependence on particle size was observed. The resistivity decreases with increasing carbonization temperature and most of the decrease takes place under 700C; between temperatures of 350C and 700C the resistivity changes from 0.35 ohm cm to 0.05 ohm cm, and from 700C to 1000C the resistivity decreases only to 0.03 ohm cm. Analyses of the volatile matter evolved from the wood chars show appreciable increase in the amount of hydrogen at carbonization temperatures above 700C.