A superconducting sample with nominal composition of Bi1.3Pb0.4V0.3Sr2Ca2Cu3Od prepared by using solid-state reaction method. DC electrical resistivity of the sample determined by using a standard four-probe technique within a temperature range of 77-300 K. Zero electrical resistivity of the sample was found at a critical temperature (Tc,zero) of 108 ± 1 K. Whereas, the onset temperature (Tc,onset) was observed at 122 ± 1 K. Temperature dependent thermoelectric power (Seebeck coefficient) of the superconducting sample was measured with a newly developed and calibrated apparatus.