Zn1-X LiXO samples have been synthesized by conventional solid state reaction method and studied their structure, grain size, and electrical properties. The crystalline grain size and lattice constants were determined from the profile of x-ray diffraction. X-ray study shows that Li is soluble in ZnO upto 30 mol.%. The approximate grain size of the crystal in the direction perpendicular to (100), (002), (101), (102) and (110) planes ranges from 45 to 56 nm. The lattice parameters of these materials are consistent with the reported values. The dc electrical conductivity measurement shows that all samples are highly resistive (~106 ohm-cm) upto a certain critical temperature (Tc) above which conductivity of the materials increases gradually. The band gap energy (3.19-3.5 eV) calculated from conductivity measurement is comparable to the optical band gap of ZnO crystal, which reveals that after Tc, electron transition occurs from valence band to conduction band only.