Two series of Composite Polymeric Membranes (CPMs) based on Poly (Vinyl Chloride) (PVC) and inorganic filler were prepared by solvent casting method, using Tetrahydrofuran (THF) and a mixture of THF and Dimethylsulfoxide (DMSO). The different percentages (5-35 %) of Bentonite clay (79-89 mesh, ASTM) filler were used. The physicochemical parameters of the CPMs i.e. degree of perpendicular swelling, liquid uptake (water, methanol, and ethanol), density, ion adsorption capacity (IAC), porosities, electrical resistivity, and conductivities were evaluated. The Type-B CPMs cast with THF and DMSO mixture have greater values of the above parameters except density than the Type-A CPMs cast with THF only. The CPMs having more filler show more liquid uptake. The uptake of Water, ethyl alcohol (EtOH), 5M methanol and methanol (MeOH) in Type-B CPMs was found 8–11, 10.12–12.83, 3.40–10.88 and 11.37–15.25 times more than Type-A CPMs. Proton ion adsorption capacity of Type-B CPMs was calculated 2.83 to 8.4 times more than Type-A CPMs. The porosity range of Type-A CPMs was observed 0.0377 to 0.093, 0.0227 to 0.0909, 0.02 to 0.0408 and 0.0476 to 0.1112; whereas porosity range in Type-B CPMs were noted 0.1955 to 0.4919, 0.1477 to 0.4835, 0.115 to 0.2554 and 0.1177 to 0.4447 in deionized water, EtOH, 5M MeOH and MeOH respectively The conductivity of Type-B CPMs was 150-333 times greater than Type-A CPMs. These all characteristics were compared with pure Poly (Vinyl Chloride) membrane (prepared and studied by same method) cast with DMSO and without DMSO.