Medium carbon steel strips containing 0.35% carbon were hot-dip-aluminized in pure AI and AI-Cualloys. An iron-aluminum interlayer, which is brittle in nature, developed at the interface between the melt and the steel substrate. Cu additions (4~16% by weight) in Al affected the growth rate of interlayer as well as the hardness and oxidation resistance of the aluminized surface. These effects were examined by using scanning electron microscopy, XRD (X-Ray Diffraction), and TGA (Thermal Gravimetric Analysis). In HAD (Hot Dip Aluminizing) with pure aluminum, the interlayer was “thick” and exhibited a finger-like growth into steel substrate. While aluminizing in AI-Cu alloys, the thickness of the interlayer decreased consistently by gradually increasing the addition of Cu content in AI from 4~16%. Further, the addition of Cu beyond 12% transformed finger-like interface into nearly smooth interface. XRD analysis revealed that due to Cu addition, the tetragonal phases, AI2 Cu and AI7Cu2 Fe formed in surface coating in addition to FeAI3 and Fe2AI5, which generally form in steel HDA in pure AI. Their formation caused to reduce the growth of interlayer. Steel surface aluminized in AI. Their formation caused to reduce the growth of interlayer. Steel surface aluminized in AI-Cu alloys exhibited better hardness than of aluminized in pure AI and AI-Si alloys and also expressed excellent oxidation resistance up to 632oC.